Blomlöf J, Cederlund A, Jonsson B, Ohlson N G
Department of Basic Oral Sciences, School of Dentistry, Karolinska Institute, PO Box 4064, SE-141 04 Huddinge, Sweden.
Quintessence Int. 2001 Oct;32(9):711-5.
The purpose of the present study was to compare ethylenediaminetetraacetic acid conditioning and phosphoric acid conditioning of dentin in combination with two principally different commercial dentin bonding systems.
Twenty-one extracted human third molars were used. All teeth were caries free, and no teeth were root filled. In total, 29 pairs of dentin surfaces were obtained from 21 teeth. One dentin surface in each pair was etched with a 32% phosphoric acid gel for 15 seconds, and the opposite surface was etched with a 24% ethylenediaminetetraacetic acid gel for 3 minutes. One experimental group of 15 dentin surface pairs was subsequently bonded with All-Bond 2, a two-component system, and the other group of 14 pairs was bonded with Prime & Bond NT, a one-bottle adhesive. A flowable resin composite was inserted in the experimental cavity and light cured. Shear bond strength testing was performed according to the protocol of the International Organization for Standardization.
The combination of conditioning with ethylenediaminetetraacetic acid and bonding with All-Bond 2 was significantly better than all other combinations, providing a shear bond strength that was 61% to 123% greater.
Use of ethylenediaminetetraacetic acid in combination with All-Bond 2 resulted in a significantly greater bond strength to dentin than did conventional acid etching.
本研究旨在比较乙二胺四乙酸(EDTA)处理和磷酸处理牙本质,并结合两种主要不同的商用牙本质粘结系统的效果。
使用21颗拔除的人类第三磨牙。所有牙齿均无龋坏,且无根充情况。从21颗牙齿共获得29对牙本质表面。每对中的一个牙本质表面用32%的磷酸凝胶蚀刻15秒,相对的表面用24%的乙二胺四乙酸凝胶蚀刻3分钟。一组15对牙本质表面随后用双组分系统All-Bond 2粘结,另一组14对用单瓶粘结剂Prime & Bond NT粘结。将可流动树脂复合材料填入实验窝洞并光固化。根据国际标准化组织的方案进行剪切粘结强度测试。
乙二胺四乙酸处理与All-Bond 2粘结的组合明显优于所有其他组合,其剪切粘结强度高出61%至123%。
与传统酸蚀相比,乙二胺四乙酸与All-Bond 2联合使用能显著提高与牙本质的粘结强度。