Thomas I M
Appl Opt. 1992 Oct 1;31(28):6145-9. doi: 10.1364/AO.31.006145.
Coatings of refractive index that vary between 1.22 and 1.44 were prepared from combinations of a colloidal silica suspension and a polysiloxane solution. The polysiloxane acted both as a binder and a filler for the colloidal silica particles. Increasing ratios gave coatings of lower porosity, hence higher refractive index, and better abrasion resistance. This variation in refractive index allowed highefficiency quarter-wave antireflection coatings to be prepared on substrates whose index varied from 1.45 to 2.1. The laser damage thresholds of all the coatings were >50 J/cm(2) at a wavelength of 1.06 microm with a 10-ns pulse length.