Habibzadeh Sareh, Safaeian Shima, Behruzibakhsh Marjan, Kaviyani Parisa, Kharazifard Mohamadjavad
Assistant Professor, Department of Prosthodontics, School of Dentistry, International Campus, Tehran University of Medical Sciences, Tehran, Iran.
Assistant Professor, Department of Dental Materials, School of Dentistry, Tehran University of Medical Sciences, Tehran, Iran.
J Dent (Tehran). 2016 Jun;13(3):193-198.
This study aimed to assess the effect of storage time and temperature on dimensional stability of impressions made with Cavex Outline zinc oxide impression paste.
A round stainless steel mold with five grooves (three horizontal and two vertical) was used in this in-vitro experimental study. Cavex Outline impression paste was prepared according to the manufacturer's instructions and applied to the mold. The mold was placed on a block and stored at 35°C and 100% humidity for setting. The impressions were poured with stone immediately and also after 30, 120, 240 and 420 minutes and 24 hours. The distance between the vertical lines on the casts was measured and compared with that in the immediately poured cast.
Storage in a refrigerator and at room temperature for zero to seven hours had no significant effect on dimensional stability of the impressions; however, 24 hours of storage in a refrigerator or at room temperature decreased the dimensional stability of Cavex Outline (P=0.001). Also, a significant association was found between dimensional changes following 24 hours of storage in a refrigerator (4°C) and at room temperature (23°C; P<0.01).
The optimal pouring time of Cavex Outline impressions with stone is between zero to seven hours, and 24 hours of storage significantly decreases the dimensional stability.
本研究旨在评估储存时间和温度对使用Cavex Outline氧化锌印模膏制作的印模尺寸稳定性的影响。
本体外实验研究使用了一个带有五条凹槽(三条水平和两条垂直)的圆形不锈钢模具。按照制造商的说明制备Cavex Outline印模膏并应用于模具。将模具放置在一个块上,在35°C和100%湿度下储存以进行凝固。印模立即灌注石膏,以及在30、120、240和420分钟及24小时后灌注石膏。测量铸型上垂直线之间的距离,并与立即灌注石膏的铸型进行比较。
在冰箱和室温下储存零至七小时对印模的尺寸稳定性没有显著影响;然而,在冰箱或室温下储存24小时会降低Cavex Outline的尺寸稳定性(P = 0.001)。此外,发现在4°C冰箱和23°C室温下储存24小时后的尺寸变化之间存在显著关联(P < 0.01)。
Cavex Outline印模与石膏的最佳灌注时间为零至七小时,储存24小时会显著降低尺寸稳定性。