Suppr超能文献

使用国际牙科联盟(FDI)标准对瓷贴面进行的两年评估。

Two-year evaluation of porcelain laminate veneers using FDI criteria.

作者信息

Yıldırım Bengisu, Recen Duygu, Paken Gamze

机构信息

Department of Prosthodontics, Faculty of Dentistry, University of Uşak, Usak, Turkey.

İzmir Torbalı Oral and Dental Health Center, İzmir, Turkey.

出版信息

J Prosthodont. 2023 Dec;32(9):854-860. doi: 10.1111/jopr.13641. Epub 2023 Feb 6.

Abstract

PURPOSE

The use of porcelain laminate veneers (PLVs) is a minimally invasive technique that is often used in restorative dentistry due to esthetic considerations. The aim of this study was to evaluate PLVs according to the Fédération Dentaire Internationale (FDI) World Dental Federation clinical criteria.

MATERIALS AND METHODS

This clinical study included 11 patients (7 female and 4 male) who had been admitted to the Uşak University Faculty of Dentistry between February 2019 and February 2021. Before taking part in the study, patients were informed about alternative treatment procedure options. A total of 30 PLVs were fabricated and cemented, and patients were evaluated according to the FDI criteria (with a follow-up after 2 years).

RESULTS

Restorations were evaluated by two trained researchers. During the follow-up evaluation, no fractures or cracks were observed in any restoration. Further, 73% (n = 22) of the PLVs had perfect marginal adaptation and only 27% (n = 8) had small marginal fractures that could be removed by polishing. Moreover, 57% (n = 17) of the PLVs were evaluated as a good color match (no difference in shade and/or translucency), whereas 33% (n = 13) had only minor deviations. In periodontal examinations, 23% (n = 7) of the PLVs had no plaque, inflammation, or pockets, whereas 77% (n = 23) had minor plaque inflammation and no pocket development.

CONCLUSIONS

As there were no fractures, fails, or need for removal of the restorations after 2 years, PLVs showed clinically satisfactory performance. The performance of PLVs can be considered highly favorable due to the minimally invasive and periodontally-compatible nature, with a good color match when carefully planned.

摘要

目的

瓷贴面(PLV)的使用是一种微创技术,出于美学考虑,常用于修复牙科。本研究的目的是根据国际牙科联合会(FDI)世界牙科联盟的临床标准评估瓷贴面。

材料与方法

本临床研究纳入了2019年2月至2021年2月期间在屈塔希亚大学牙科学院就诊的11例患者(7例女性,4例男性)。在参与研究之前,向患者告知了替代治疗程序选项。共制作并粘结了30颗瓷贴面,并根据FDI标准对患者进行评估(随访2年)。

结果

修复体由两名经过培训的研究人员进行评估。在随访评估期间,未观察到任何修复体出现骨折或裂缝。此外,73%(n = 22)的瓷贴面边缘贴合完美,只有27%(n = 8)有小的边缘骨折,可通过抛光去除。此外,57%(n = 17)的瓷贴面颜色匹配良好(色调和/或透明度无差异),而33%(n = 13)仅有轻微偏差。在牙周检查中,23%(n = 7)的瓷贴面没有菌斑、炎症或牙周袋,而77%(n = 23)有轻微的菌斑炎症且没有牙周袋形成。

结论

由于2年后没有骨折、失败或需要拆除修复体的情况,瓷贴面在临床上表现出令人满意的性能。由于其微创性和牙周兼容性,精心设计时颜色匹配良好,瓷贴面的性能可被认为非常理想。