光固化时间和光照面形状对托槽与牙釉质间黏结强度和单体转化率的影响。

Effect of time and photoactivated face on bond strength of brackets and on degree of monomer conversion.

机构信息

Department of Dentistry, Federal University of Rio Grande do Norte - UFRN, Natal, RN, Brazil.

Graduate Program in Dental Sciences, Department of Dentistry, Federal University of Rio Grande do Norte - UFRN, Natal, RN, Brazil.

出版信息

Clin Oral Investig. 2024 Aug 5;28(8):465. doi: 10.1007/s00784-024-05854-5.

Abstract

OBJECTIVE

To evaluate the effect of four different photoactivation protocols (according to "photoactivated faces" - mesial/distal, cervical/incisal or center - and "photoactivation time" - 6-3 s) of a high-power photo activator (Valo Cordless-Ultradent) on the shear bond strength (SBS) between metal brackets and dental enamel and on the degree of conversion (DC) of an orthodontic resin.

MATERIALS AND METHODS

40 bovine incisor crowns were randomly assigned to 4 groups (n = 10). The brackets were bonded with Transbond XT resin using 4 protocols according to the "photoactivation protocol" factor (which was subdivided into photoactivated faces and photoactivation time): V3C = 3 s + center; V6C = 6 s + center; V3M3D = 3 s on mesial + 3 s on distal; V3C3I = 3 s on cervical + 3 s on incisal. All the samples were stored for 4 months (water,37ºC) and then subjected to a SBS test (100KgF,1 mm/min). 40 resin discs were made to evaluate the monomer degree of conversion. Data from the SBS and DC were assessed by One-way ANOVA and Tukey's test (5%). Bond failures were analyzed according to the Adhesive Remnant Index (ARI) and evaluated by the Kruskal-Wallis test (5%).

RESULTS

There was a statistically significant difference (p = 0.008) in the One-way ANOVA result for SBS values between all groups, but the protocols showed statistically similar results (p ≥ 0.05-Tukey's tests) concerning the photoactivated faces (V6C, V3M3D and V3C3I) and photoactivation time (V3C and V6C) factors individually. There was no statistically significant difference (p ≥ 0.05) in the One-way ANOVA result for DC values.

CONCLUSION

The SBS and DC values will vary depending on the protocol applied.

CLINICAL RELEVANCE

It is possible to maintain the bracket fixation quality with the use of a high-power LED photo activator associated with a shorter photoactivation time. However, it is assumed that not all types of protocols that might be applied will provide quality bonding, such as V3C, V3M3D and V3C3I, which may - depending on the SBS and DC values - affect the final treatment time, due to brackets debonding, or increase of possibility of damage to dental enamel during bracket removal. Clinical studies are suggested to confirm the hypotheses of this research.

摘要

目的

评估高功率光激活器(Valo Cordless-Ultradent)的四种不同光激活方案(根据“光激活面”——近远中/切颈——和“光激活时间”——6-3 s)对金属托槽和牙釉质之间的剪切结合强度(SBS)和正畸树脂的转化率(DC)的影响。

材料和方法

将 40 个牛切牙冠随机分为 4 组(n=10)。根据“光激活方案”因素(分为光激活面和光激活时间),使用 Transbond XT 树脂将托槽粘合:V3C=3 s+中心;V6C=6 s+中心;V3M3D=3 s 近中+3 s 远中;V3C3I=3 s 颈侧+3 s 切侧。所有样本均在 37°C 水中储存 4 个月,然后进行 SBS 测试(100 Kgf,1 mm/min)。制作 40 个树脂圆盘以评估单体转化率。SBS 和 DC 的数据通过单因素方差分析和 Tukey 检验(5%)进行评估。根据黏附残余指数(ARI)分析黏结失败情况,并通过 Kruskal-Wallis 检验(5%)进行评估。

结果

SBS 值的单因素方差分析结果在各组之间存在统计学差异(p=0.008),但 V6C、V3M3D 和 V3C3I 三个光激活面和 V3C 和 V6C 两个光激活时间因素的方案在统计学上结果相似(p≥0.05-Tukey 检验)。DC 值的单因素方差分析结果无统计学差异(p≥0.05)。

结论

SBS 和 DC 值将取决于所应用的方案。

临床相关性

使用高功率 LED 光激活器结合更短的光激活时间,仍可以保持托槽的固定质量。然而,并非所有可能应用的方案都能提供高质量的黏结,如 V3C、V3M3D 和 V3C3I,这可能会——根据 SBS 和 DC 值——影响最终治疗时间,因为托槽可能会脱落,或者在去除托槽时增加牙釉质损坏的可能性。建议进行临床研究以证实本研究的假设。