Bansal R K, Tewari U S, Singh P, Murthy D V
Department of Chemistry, Indian Institute of Technology, ITMMEC, Indian Institute of Technology, New Delhi, India.
J Oral Rehabil. 1997 Jan;24(1):76-9. doi: 10.1046/j.1365-2842.1997.00454.x.
Zinc oxide, the inorganic component of polycarboxylate cement, was mixed with talc in various proportions from 10% to 50%. These powder mixtures were spatulated with poly(acrylic acid) in three powder to liquid (P/L) ratios of 1:1, 1.5:1 and 2:1 (w/w). Properties such as setting time and compressive and diametral tensile strengths of the resultant cements were determined. It was observed that the setting time of the resultant cements increased with increasing talc content. The compressive and diametral tensile strengths also increased by approximately 54% with a 10% concentration of talc.
聚羧酸锌水门汀的无机成分氧化锌与滑石粉按10%至50%的不同比例混合。这些粉末混合物与聚丙烯酸按1:1、1.5:1和2:1(重量/重量)三种粉液比进行调拌。测定了所得水门汀的凝固时间、抗压强度和径向拉伸强度等性能。观察到所得水门汀的凝固时间随滑石粉含量的增加而延长。滑石粉浓度为10%时,抗压强度和径向拉伸强度也提高了约54%。