Suppr超能文献

不同修整方案后不同类型可流动修复树脂的三维表面轮廓分析

Three-dimensional surface profile analysis of different types of flowable restorative resins following different finishing protocols.

作者信息

Yazici A Rüya, Müftü Ali, Kugel Gerard

机构信息

Department of Conservative Dentistry, Faculty of Dentistry, Hacettepe University, Ankara, Turkey.

出版信息

J Contemp Dent Pract. 2007 Jul 1;8(5):9-17.

Abstract

AIM

The aim of this study was to investigate the surface roughness of different types of flowable restorative resins and compare the effectiveness of diamond finishing burs followed by aluminum oxide discs with aluminum oxide discs alone in producing smooth surfaces.

METHODS AND MATERIALS

Twenty-four specimens (10 mm X 2 mm) for each flowable resin (flowable microhybrid composite, flowable liquid microhybrid composite, flowable compomer, and flowable ormocer) were fabricated in an acrylic mold and randomly assigned to three groups. In group I samples were left undisturbed after the removal of a Mylar strip (control). In group II samples were polished with diamond finishing burs, followed by aluminum oxide discs. In group III samples were finished with only aluminum oxide discs. The mean surface roughness (Ra, microm) was determined with 3-D non-contact interferometry. Data were subjected to one way analysis of variance (ANOVA), and post hoc comparison was accomplished using Tukey's HSD.

RESULTS

Although significant differences in surface roughness (Ra) values were observed among the materials using a Mylar strip (control), no significant differences between restorative materials were found when all finishing/polishing methods were combined. For all flowable restorative resins tested, the Mylar strip produced surfaces smoother than those produced by a diamond finishing bur followed by a disc or by using discs alone. Surface roughness values were statistically similar for a diamond finishing bur followed by a disc and for disc treated surfaces within each material except for Dyract Flow, a flowable compomer.

CONCLUSION

Although the surface roughness of flowable restorative resins differs among the types, this difference can be overcome with different finishing/polishing methods.

摘要

目的

本研究旨在调查不同类型的可流动修复树脂的表面粗糙度,并比较先用金刚石精修钻再用氧化铝盘与仅用氧化铝盘在产生光滑表面方面的效果。

方法和材料

在丙烯酸模具中为每种可流动树脂(可流动微混合复合材料、可流动液体微混合复合材料、可流动复合体和可流动有机陶瓷)制作24个样本(10毫米×2毫米),并随机分为三组。在第一组中,移除聚酯薄膜条后样本保持原状(对照)。在第二组中,先用金刚石精修钻抛光样本,然后用氧化铝盘抛光。在第三组中,仅用氧化铝盘对样本进行修整。使用三维非接触干涉测量法测定平均表面粗糙度(Ra,微米)。数据进行单因素方差分析(ANOVA),并使用Tukey's HSD进行事后比较。

结果

尽管使用聚酯薄膜条(对照)时各材料之间在表面粗糙度(Ra)值上存在显著差异,但当所有修整/抛光方法结合使用时,修复材料之间未发现显著差异。对于所有测试的可流动修复树脂,聚酯薄膜条产生的表面比先用金刚石精修钻再用盘或仅用盘产生的表面更光滑。除了可流动复合体Dyract Flow外,对于每种材料,先用金刚石精修钻再用盘处理的表面和仅用盘处理的表面的粗糙度值在统计学上相似。

结论

尽管不同类型的可流动修复树脂的表面粗糙度有所不同,但这种差异可以通过不同的修整/抛光方法来克服。