Johnson Glen H, Lepe Xavier, Zhang Hai, Wataha John C
Department of Restorative Dentistry, School of Dentistry, University of Washington, Seattle, Wash. 98195-7456, USA.
J Am Dent Assoc. 2009 Sep;140(9):1125-36. doi: 10.14219/jada.archive.2009.0340.
New types of crown and bridge cement are in use by practitioners, and independent studies are needed to assess their effectiveness. The authors conducted a study in three parts (study A, study B, and study C) and to determine how well these new cements retain metal-ceramic crowns.
The authors prepared teeth with a 20-degree taper and a 4-millimeter length. They cast high-noble metal-ceramic copings, then fitted and cemented them with a force of 196 newtons. The types of cements they used were zinc phosphate, resin-modified glass ionomer, conventional resin and self-adhesive modified resin. They thermally cycled the cemented copings, then removed them. They recorded the removal force and calculated the stress of dislodgment by using the surface area of each preparation. They used a single-factor analysis of variance to analyze the data (alpha = .05).
The mean stresses necessary to remove crowns, in megapascals, were 8.0 for RelyX Luting (3M ESPE, St. Paul, Minn.), 7.3 for RelyX Unicem (3M ESPE), 5.7 for Panavia F (Kuraray America, New York) and 4.0 for Fuji Plus (GC America, Alsip, Ill.) in study A; 8.1 for RelyX Luting, 2.6 for RelyX Luting Plus (3M ESPE) and 2.8 for Fuji CEM (GC America) in study B; and 4.9 for Maxcem (Kerr, Orange, Calif.), 4.0 for BisCem (Bisco, Schaumburg, Ill.), 3.7 for RelyX Unicem Clicker (3M ESPE), 2.9 for iCEM (Heraeus Kulzer, Armonk, N.Y.) and 2.3 for Fleck's Zinc Cement (Keystone Industries, Cherry Hill, N.J.) in study C.
Powder-liquid versions of new cements were significantly more retentive than were paste-paste versions of the same cements. The mean value of crown removal stress for the new self-adhesive modified-resin cements varied appreciably among the four cements tested. All cements retained castings as well as or better than did zinc phosphate cement.
Powder-liquid versions of cements, although less convenient to mix, may be a better clinical choice when crown retention is an issue. All cements tested will retain castings adequately on ideal preparations because the corresponding removal stresses are comparable with or higher than those associated with zinc phosphate. Powder-liquid resin-modified glass ionomer cement, selected self-adhesive modified-resin cements and conventional resin cements provide additional retention when desired.
从业者正在使用新型的冠桥粘结剂,需要进行独立研究以评估其有效性。作者进行了一项分为三个部分(研究A、研究B和研究C)的研究,以确定这些新型粘结剂对金属烤瓷冠的固位效果如何。
作者制备了锥度为20度、长度为4毫米的牙齿。他们铸造了高贵金属烤瓷内冠,然后以196牛顿的力进行就位和粘结。他们使用的粘结剂类型有磷酸锌、树脂改性玻璃离子水门汀、传统树脂和自粘结改性树脂。他们对粘结好的内冠进行热循环处理,然后将其去除。他们记录去除力,并通过使用每个制备体的表面积计算脱位应力。他们使用单因素方差分析来分析数据(α = 0.05)。
在研究A中,以兆帕为单位,去除冠所需的平均应力分别为:3M ESPE公司(明尼苏达州圣保罗)的RelyX Luting为8.0,3M ESPE公司的RelyX Unicem为7.3,可乐丽美国公司(纽约)的Panavia F为5.7,GC美国公司(伊利诺伊州阿尔西普)的Fuji Plus为4.0;在研究B中,3M ESPE公司的RelyX Luting为8.1,3M ESPE公司的RelyX Luting Plus为2.6,GC美国公司的Fuji CEM为2.8;在研究C中,克尔公司(加利福尼亚州奥兰治)的Maxcem为4.9,必思科公司(伊利诺伊州绍姆堡)的BisCem为4.0,3M ESPE公司的RelyX Unicem Clicker为3.7,贺利氏古莎公司(纽约州阿蒙克)的iCEM为2.9,基石工业公司(新泽西州樱桃山)的弗莱克磷酸锌粘结剂为2.3。
新型粘结剂的粉液剂型比相同粘结剂的糊剂剂型具有显著更高的固位力。在所测试的四种新型自粘结改性树脂粘结剂中,冠去除应力的平均值差异明显。所有粘结剂对铸件的固位效果与磷酸锌粘结剂相同或更好。
粘结剂的粉液剂型虽然混合不太方便,但在冠固位是一个问题时可能是更好的临床选择。所有测试的粘结剂在理想的制备体上都能充分固位铸件,因为相应的去除应力与磷酸锌粘结剂相当或更高。当需要时,粉液型树脂改性玻璃离子水门汀、选定的自粘结改性树脂粘结剂和传统树脂粘结剂可提供额外的固位力。