Nair Anoop, Regish K M, Patil N P, Prithviraj D R
MDS, Senior lecturer, Dept. of Prosthodontics. Govt. Dental College and Research Institute, Bangalore. Victoria Hospital Campus, Fort, Bangalore, India. 560002.
BDS (MDS),Post Graduate, Dept. of Prosthodontics. Govt. Dental College and Research Institute, Bangalore. Victoria Hospital Campus, Fort, Bangalore, India. 560002.
J Clin Exp Dent. 2012 Apr 1;4(2):e91-6. doi: 10.4317/jced.50714. eCollection 2012 Apr.
The resin-bonded fixed partial dentures have gained immense popularity in recent years as they are more conservative, esthetic, economic and easily fabricated. However debonding is considered the most common cause of failure of resin bonded prosthesis. The objective of the study were to compare the effects of different groove lengths and thickness of retainers on retention of maxillary anterior base metal resin bonded retainers.
Twenty five metal dies of maxillary central incisor duplicated from pure typhodont teeth (maxillary left central incisors) prepared to receive retainer for resin bonded fixed partial denture having different test designs were made. Five test groups were made with each group having five specimens. Two groups were having preparation depth of 0.5mm and retention groove lengths of 3mm and 5mm. Two groups had preparation depths of 0.3 and 0.7mm with no groove preparation with retainer thickness of 0.3 and 0.7mm respectively. Fifth group with no groove preparation and preparation depth of 0.5mm was kept as control for all the groups. All the specimens were cemented using calibra (Dentsply) resin cement. Each specimen was subjected to tensile loading in vertical direction on universal testing machine (Instron 5569) at a crosshead speed of 1mm/min. \
Groups with 5mm and 3mm groove length recorded higher mean vertical forces when compared to the group with no groove preparation. Group with 5mm groove length showed highest mean vertical forces. The group with 0.7mm retainer recorded higher mean vertical force values when compared to groups with 0.5mm and 0.3mm retainer thickness. Group with 0.3mm retainer thickness recorded the least mean vertical force value.
Placement of the grooves increased the retention values almost 2 ½ times than the grooveless preparation and as the thickness of the retainers increased retention values also increased. Retention value was directly proportional to the groove length and retainer thickness. Key words:Groove length, retainer thickness, resin bonded bridges.
近年来,树脂粘结固定局部义齿因其更保守、美观、经济且易于制作而广受欢迎。然而,脱粘被认为是树脂粘结修复体失败的最常见原因。本研究的目的是比较不同沟长度和固位体厚度对上颌前牙金属树脂粘结固位体固位力的影响。
从纯藻酸盐牙(上颌左中切牙)复制出25个上颌中切牙金属代型,制备成可容纳具有不同测试设计的树脂粘结固定局部义齿固位体。分为五个测试组,每组有五个标本。两组制备深度为0.5mm,固位沟长度分别为3mm和5mm。两组制备深度分别为0.3mm和0.7mm,不制备沟,固位体厚度分别为0.3mm和0.7mm。第五组不制备沟,制备深度为0.5mm,作为所有组的对照。所有标本均使用卡利布拉(登士柏)树脂水门汀粘结。每个标本在万能试验机(英斯特朗5569)上以1mm/min的十字头速度在垂直方向上进行拉伸加载。
与未制备沟的组相比,沟长度为5mm和3mm的组记录到更高的平均垂直力。沟长度为5mm的组显示出最高的平均垂直力。与固位体厚度为0.5mm和0.3mm的组相比,固位体厚度为0.7mm的组记录到更高的平均垂直力值。固位体厚度为0.3mm的组记录到的平均垂直力值最小。
制备沟可使固位力值比未制备沟增加近2.5倍,并且随着固位体厚度的增加,固位力值也增加。固位力值与沟长度和固位体厚度成正比。关键词:沟长度、固位体厚度、树脂粘结桥