Begazo Catherine C, de Boer Hielke D, Kleverlaan Cornelis J, van Waas Marinus A J, Feilzer Albert J
Department of Dental Material Science, ACTA, Louwesweg 1, 1066 EA, Amsterdam, The Netherlands.
Dent Mater. 2004 Dec;20(10):901-7. doi: 10.1016/j.dental.2003.10.011.
The aim of this study was to find the optimal choice of luting cement to Synthoceram, an aluminum oxide-reinforced glass ceramic material. The bond strength of five different commercial luting cements to the ceramic material was evaluated. The effect of surface treatments, etching, sandblasting, silanizing, and combinations of these treatments was also investigated.
Shear bond strength tests were performed using the ceramic material as substrate with each of the luting cements. Cements rods were prepared on pre-treated ceramic surfaces. The shear bond strength was determined 24 h after cementation. The effect of surface treatments: etching, sandblasting, and sandblasting followed by etching, respectively, on the morphology of the material, was investigated with SEM.
The shear bond strength increases significantly from Ketac Cem, Rely X Luting, Fuji Plus, Panavia F to Xeno Cem. The surface treatments etching and/or sandblasting followed by silanization generally provide the highest bond strength values.
Based on the results of this study, the use of resin composite based cements is preferred for cementation of an all-ceramic restoration with an aluminum oxide-reinforced glass ceramic base. Surface treatment of etching and/or sandblasting followed by silanization is recommended.
本研究旨在找出用于Synthoceram(一种氧化铝增强玻璃陶瓷材料)的最佳粘结水门汀。评估了五种不同市售粘结水门汀与该陶瓷材料的粘结强度。还研究了表面处理(蚀刻、喷砂、硅烷化以及这些处理的组合)的效果。
使用陶瓷材料作为基材,对每种粘结水门汀进行剪切粘结强度测试。在预处理的陶瓷表面制备水门汀棒。粘结后24小时测定剪切粘结强度。用扫描电子显微镜研究表面处理(分别为蚀刻、喷砂以及喷砂后蚀刻)对材料形态的影响。
从Ketac Cem、Rely X Luting、Fuji Plus、Panavia F到Xeno Cem,剪切粘结强度显著增加。蚀刻和/或喷砂后进行硅烷化的表面处理通常能提供最高的粘结强度值。
基于本研究结果,对于氧化铝增强玻璃陶瓷基底的全瓷修复体粘结,首选使用树脂复合材料基水门汀。建议采用蚀刻和/或喷砂后进行硅烷化的表面处理。