Cadenaro Milena, Fontanive Luca, Navarra Chiara Ottavia, Gobbi Pietro, Mazzoni Annalisa, Di Lenarda Roberto, Tay Franklin R, Pashley David H, Breschi Lorenzo
Department of Medical Sciences, University of Trieste, Piazza dell'Ospitale 1, I-34129 Trieste, Italy.
Department of Medical Sciences, University of Trieste, Piazza dell'Ospitale 1, I-34129 Trieste, Italy.
Dent Mater. 2016 Apr;32(4):492-8. doi: 10.1016/j.dental.2015.12.006. Epub 2016 Jan 5.
1-ethyl-3-(3-dimethylaminopropyl) carbodiimide hydrochloride (EDC) has been shown to cross-link dentin type I collagen. Increased cross-linking usually elevates the glass transition temperature of polymers. The aim of this study was to evaluate the cross-linking reaction promoted by EDC in different aqueous concentrations by measuring the thermal denaturation temperature (Td) of human dentin collagen.
The Td of dehydrated collagen and of insoluble dentin matrix collagen immersed in 0.5M or 1M EDC aqueous solution for different treatment times was obtained using a Differential Scanning Calorimeter (DSC). Specimens were also analyzed by Energy Dispersive X-Ray Spectroscopy.
EDC-treated dentin collagen showed a significantly higher Td than the untreated specimens when immersed in either 0.5M EDC or 1M EDC for 10min or longer (p<0.05). EDC-treated dentin collagen showed an increase of sulfur and chloride, not detectable in EDC-untreated dentin specimens. Conversely, the relative amount of carbon, nitrogen and oxygen was not modified by treatments.
EDC-treated dentin collagen showed a higher Td than the untreated control at all tested concentrations and immersion times. A higher Td can be considered an indirect indicator of a more resistant and highly cross-linked collagen network. More data are needed to confirm these results.
已证实盐酸1-乙基-3-(3-二甲基氨基丙基)碳二亚胺(EDC)可交联牙本质I型胶原。交联增加通常会提高聚合物的玻璃化转变温度。本研究的目的是通过测量人牙本质胶原的热变性温度(Td)来评估不同水溶液浓度的EDC促进的交联反应。
使用差示扫描量热仪(DSC)获得脱水胶原以及浸入0.5M或1M EDC水溶液中不同处理时间的不溶性牙本质基质胶原的Td。还通过能量色散X射线光谱对标本进行分析。
当浸入0.5M EDC或1M EDC中10分钟或更长时间时,经EDC处理的牙本质胶原显示出比未处理标本显著更高的Td(p<0.05)。经EDC处理的牙本质胶原显示硫和氯增加,在未用EDC处理的牙本质标本中未检测到。相反,碳、氮和氧的相对含量未因处理而改变。
在所有测试浓度和浸泡时间下,经EDC处理的牙本质胶原显示出比未处理对照更高的Td。更高的Td可被视为更具抗性和高度交联的胶原网络的间接指标。需要更多数据来证实这些结果。