Suppr超能文献

一种造型树脂和热循环对不同树脂复合材料的表面硬度、粗糙度及颜色的影响。

The effect of a modeling resin and thermocycling on the surface hardness, roughness, and color of different resin composites.

作者信息

Tuncer Safa, Demirci Mustafa, Tiryaki Murat, Unlü Nimet, Uysal Ömer

机构信息

Department of Conservative Dentistry, Faculty of Dentistry, Istanbul University, Istanbul, Turkey.

出版信息

J Esthet Restor Dent. 2013 Dec;25(6):404-19. doi: 10.1111/jerd.12063. Epub 2013 Oct 31.

Abstract

STATEMENT OF PROBLEM

The application of modeling resin could affect the surface quality and color of resin composites.

PURPOSE

To evaluate the effects of modeling resin on the microhardness, roughness, and color of composite restorations, with and without thermocycling.

METHODS

Sixty disc-shaped specimens for each resin composite were prepared in three groups: Group 1: A resin composite disc was cured against a polyester matrix and finished/polished; Group 2: A composite instrument was wetted with Bisco Modeling Resin (Bisco, Schaumburg, IL, USA) to smooth the composite surface, which was cured against a polyester matrix and finished/polished; Group 3: A composite instrument was wetted with modeling resin to smooth the composite surface, which was cured against a polyester matrix. Microhardness, roughness, and color were measured 24 hours after curing and after 10,000 thermocycles.

RESULTS

Modeling resin significantly influenced the microhardness of GrandioSO (Voco, Cuxhaven, Germany) and Gradia Direct Posterior (GC America, Alsip, IL, USA), and the surface roughness of GrandioSO, Filtek Silorane (3M ESPE, St Paul, MN, USA), and Aelite All Purpose Body (Bisco) (p < 0.05). The microhardness of the Group 1 resin composites was affected by thermocycling (p < 0.05); however, thermocycling had no significant effect on surface roughness (p > 0.05). Tested composites showed clinically perceptible color changes after thermocycling. In Group 1, Filtek Ultimate (3M ESPE) showed the lowest color change (p < 0.05), and in Group 2, Filtek Silorane showed the highest significant color changes (p < 0.05).

CONCLUSIONS

Modeling resin did not affect the microhardness, surface roughness, and color of Aelite LS Posterior (Bisco), Filtek Ultimate (3M ESPE), and Clearfil Majesty Esthetic (Kuraray Medical Inc, Tokyo, Japan) specimens. Also, thermocycling process only affected microhardness of tested resin composites.

CLINICAL SIGNIFICANCE

The effect of modeling resin on surface microhardness, roughness, and color stability of composite materials depends on the type of resin composite. In clinical practice, the adverse effects of modeling resin might be alleviated by a proper finishing and polishing procedure.

摘要

问题陈述

造型树脂的应用可能会影响树脂复合材料的表面质量和颜色。

目的

评估造型树脂对复合修复体的显微硬度、粗糙度和颜色的影响,以及有无热循环的情况。

方法

为每种树脂复合材料制备60个圆盘形试件,分为三组:第1组:将树脂复合材料圆盘在聚酯基质上固化,然后进行修整/抛光;第2组:用Bisco造型树脂(美国伊利诺伊州绍姆堡市的Bisco公司)湿润复合器械以平滑复合材料表面,在聚酯基质上固化,然后进行修整/抛光;第3组:用造型树脂湿润复合器械以平滑复合材料表面,在聚酯基质上固化。在固化24小时后以及10000次热循环后测量显微硬度、粗糙度和颜色。

结果

造型树脂显著影响了GrandioSO(德国库克斯港的Voco公司)和Gradia Direct Posterior(美国伊利诺伊州阿尔西普市的GC America公司)的显微硬度,以及GrandioSO、Filtek Silorane(美国明尼苏达州圣保罗市的3M ESPE公司)和Aelite All Purpose Body(Bisco公司)的表面粗糙度(p < 0.05)。第1组树脂复合材料的显微硬度受热循环影响(p < 0.05);然而,热循环对表面粗糙度无显著影响(p > 0.05)。经测试的复合材料在热循环后出现了临床上可察觉的颜色变化。在第1组中,Filtek Ultimate(3M ESPE公司)的颜色变化最小(p < 0.05),在第2组中,Filtek Silorane的颜色变化最为显著(p < 0.05)。

结论

造型树脂对Aelite LS Posterior(Bisco公司)、Filtek Ultimate(3M ESPE公司)和Clearfil Majesty Esthetic(日本东京的可乐丽医疗株式会社)试件的显微硬度、表面粗糙度和颜色没有影响。此外,热循环过程仅影响测试树脂复合材料的显微硬度。

临床意义

造型树脂对复合材料表面显微硬度、粗糙度和颜色稳定性的影响取决于树脂复合材料的类型。在临床实践中,适当的修整和抛光程序可能会减轻造型树脂的不良影响。