Itota Toshiyuki, Carrick Thomas E, Rusby Sandra, Al-Naimi Omar Taha, Yoshiyama Masahiro, McCabe John F
Dental Materials Science Unit, School of Dental Sciences, University of Newcastle upon Tyne, Framlington Place, NE2 4BW, Newcastle upon Tyne, UK.
J Dent. 2004 Feb;32(2):117-22. doi: 10.1016/j.jdent.2003.09.002.
The aim of this study was to investigate the quantities of total and free fluoride ions released from four resin-based composites containing fluoride (Heliomolar (HE), UniFil S (UF), Beautifil (BE) and Reactmer paste (RP)) and one glass ionomer cement (Ketac-Fil Plus Aplicap (KF)).
Five disk specimens of each material were prepared and the fluoride release was measured at 1, 2, 4, 7, 14, 21 and 28 days. The amounts of total and free fluoride ions released from materials were measured by using an ion-selective electrode (ISE) and ion chromatography (IC). Data were statistically analyzed using a t-test at a significant level of 0.05.
For HE, fluoride release is undetectable using the ISE but was detected by the IC method. There were no significant differences in the free and total fluoride ions released from UF and BE (p>0.05). For RP, the free fluoride ions were significantly lower than the total fluoride ions after 4 days (p<0.05). KF showed significant difference between total and free fluoride ions at 7 and 28 days (p<0.05).
The nature of the fluoride incorporated into dental materials affected the amounts of free and total fluoride ions released from materials.
本研究旨在调查四种含氟树脂基复合材料(贺利氏磨牙树脂(HE)、优菲树脂S(UF)、碧兰美树脂(BE)和瑞特美尔糊剂(RP))以及一种玻璃离子水门汀(伢典补牙条加强型(KF))释放的总氟离子和游离氟离子的量。
制备每种材料的五个圆盘样本,并在第1、2、4、7、14、21和28天测量氟释放量。使用离子选择电极(ISE)和离子色谱法(IC)测量材料释放的总氟离子和游离氟离子的量。数据采用t检验进行统计学分析,显著性水平为0.05。
对于HE,使用ISE无法检测到氟释放,但通过IC法检测到了。UF和BE释放的游离氟离子和总氟离子没有显著差异(p>0.05)。对于RP,4天后游离氟离子显著低于总氟离子(p<0.05)。KF在第7天和第28天的总氟离子和游离氟离子之间存在显著差异(p<0.05)。
牙科材料中所含氟的性质影响了材料释放的游离氟离子和总氟离子的量。